           EXERCISE 38 :  Pipe butt weld butt joint on MS pipe
                                      25mm o.d. 3mm w.t. position 2G vertical
                                      arc welding


            Objectives

           At the end of this exercise you shall be able to
           •  cut bevel the pipe for welding
           •  tack pipes for butt welding
           •  make root run by rotation method
           •  make filling run by rotation
           •  clean the job and inspect for defects.

           Job Sequence

           •  Cut the pipes to the given size.

           •  File pipe ends to be at right angle to the pipe axis.
           •  Grind the edges to 30° to 35” bevel maintaining 1.5 to 1.75mm root face.
           •   Remove the burrs and rust from the pipe ends.
           •   Check the perpendicularly of the work piece using the try square.

           •  Arrange the 2 pipes to form as a butt joint.
           •  Use a fixture or V profile of an angle iron to align pipes in 6G position.
              Note: Wear protective clothing (safety apparels)

           •  Switch on the machine and select a 3.15mm dia electrode for tacking and the root run and set 100 amps
              current.
           •  Put4 tacks at regular intervals adjusting 2mm root gap between the pipes using spacers.

           •  Ensure that each tack ends with a keyhole.
           •  Check and ensure that the pipes are in line after tacking.
           •  Set 110amps for a 3.15mm dia electrode for root run.
           •  Deposit the root run in flat position by rotating the pipe.

           •  Welding using the keyhole technique ensures root penetration.
           •  Remove slag from the root thoroughly.
           •  Deposit the second and third run using 3.15mm dia electrodes i.e. the same ad for the root run.
           •  Clean and inspect the joint.
              a  To ensure uniform and correct reinforcement

              b  To ensure that the weld face is free from porosity, slag inclusion, unfilled crater, overlap and edge of plate
                 melted off/insufficient throat thickness