            Construct Corner joint on MS sheet 1.6 mm
            in Vertical position by GTAW


            Objectives

           At the end of this exercise you shall be able to
           •  produce molten pool of required size by the manipulation of torch
           •  add filler metal at the required rate and place by manipulation the filler rod
           •  deposit fusion run with filler rod in flat position and maintain uniform arc travel speed
           •  clean and inspect the deposited beads for surface defects.





































           Job Sequence

           -  Cut the plate by using hacksaw cutting as per drawing
           -  Construct Lap joint on MS sheet 1.6 mm in Vertical position by GTAW
           -  Fill the crater
           -  Manipulate the torch and filler rod in the correct position with respect job

           -  Stop the weld at the left-hand edge of the joint after filling up in the crater at the end of the weld
           -  The angular distortion between the vertical and horizontal sheets of the Tee joint is automatically controlled
           -   The current set is 10 to 15 amperes
           -  At the end of the welding perform the carter filler treatment by repeating the torch switch   ON-OFF

           -  Cut the arc and hold at the finishing point unit molten metal solidifies
           -  Visual inspection: slight convexity, uniform width, uniform ripples and free from under cut at the toes of the
              weld indicate a smooth