Page 44 - CITS - Welder - Trade Practical
P. 44

WELDER - CITS




              Fig 1                                            Fig 2



















           Deslag and clean the root bead thoroughly.
           Deposit the final covering run with a 4mmø medium coated MS electrode and 160 amp current.

           Give side-to-side movement to the electrode not more than 2.5 times its dia.
           Use the same electrode angle as was used for the root bead.
              Note: Prevent the upper edge of the plate from melting off by not allowing the arc to concentrate more
              on the upper edge.
           Remove the slag with a chipping hammer.
           Clean the weld with a steel wire brush.
           Inspect the lap fillet weld (Fig 3) and ensure:


               Fig 3














           •  It has equal leg length with slight convexity

           •  The upper edge of the plate has not melted off
           •  it is free from surface defects.






















                                                           27

                                           CITS : C G & M - Welder - Exercise 6
   39   40   41   42   43   44   45   46   47   48   49